Detailing
Drawings in this guide are typical details of specific seals that have been tested. Seals that differ from these designs may have to be independently tested or assessed to ensure that specific fire ratings are achievable. Indeed, many parameters influence the fire resistance of a sealant both for linear joints and penetration seals.
The joint dimensions, both bite/width and thickness, influence the seal’s fire resistance performance. The smaller the joint width, the longer the fire resistance (integrity and insulation) could potentially be. A larger joint thickness will also increase the fire resistance. Fire rated seals can be applied on one side (single joint) of the supporting construction or on both sides (double joint). Double joints typically provide a better fire resistance. For single joints, a different behavior exists between those applied on the exposed (fire side FS) or non-exposed (non-fire side NFS) side of the wall. The joint orientation on a wall can be vertical or horizontal. Vertical joints can reach lower performance than equivalent designs in horizontal orientation due to the gravity which can accelerate any potential failure. Linear joints in a wall, in a floor or between adjacent walls or floors do not have to resist shear movement. However, when a joint is sealing a floor abutting a wall or a ceiling abutting a wall, it is necessary to test the joint under shear movement. In European testing, the shear movement is typically a static shear deformation applied on the cured joint during the fire test. This shear movement adds more severity to the testing condition.
Parameters that influence fire resistance
| Joint parameters | Construction parameters | Penetration parameters |
|---|---|---|
| Bite and thickness | Wall material and thickness | Diameter |
| Orientation (vertical / horizontal) | Backing material (MW/backer rod) | Separation (grouped/shattered) |
| Single or double joints | Support elements for backing | Sheathing material |
| Movement or static | Compression and thickness of MW | Position (corner/middle) |
All parameters of the tested system can further influence its performance. Testing in floors is much more onerous than in walls and performance reached by certain joint configurations in walls cannot be extrapolated to a floor set up. The build-up of the supporting (wall or floor) construction, including the material and its thickness, influences the overall performance of the tested system. This effect is more pronounced for the floor test. A thicker construction can limit the heat increase around the linear joints and improve fire resistance in E and I. Forming materials, such as mineral wool or backer rods, allow the liquid applied sealant to form until cure occurs. Mineral wool has inherently excellent non-combustible behavior under fire and contributes to the overall performance of the system by limiting the temperature increase of the seal. The mineral wool specifications (density, thickness, compression, potential use of metal supports) influence the result and therefore are fully part of the tested system. Backer rods made of PU and PE are alternative means to support the sealant during its cure, which will not contribute to the fire resistance of the build-up as they tend to quickly burn away, leaving the sealant exposed to the fire. Both PU and PE have a similar fire resistance, hence testing with one or the other is deemed to be equivalent and test results obtained for one option are generally accepted to cover the other material. Finally, for penetration seals specifically, the cable parameters (sheathing material, diameter, etc), the diameter of the opening (larger being more severe) as well as the position of the cables inside the opening (clustered or spread, centered or edge of the opening) can all influence the fire resistance.
Extended application rules (EN 15882)
In Europe, rules exist to extrapolate test results for different bite parameters. For linear joints and penetration seals, the European Standard EN15882 respectively part 4 and part 3 describe the principles which apply for the extension of the field of application of a specific test result.
The extended application principles common to all generic joint seal types are as follows:
| Component | Variation | Rules |
|---|---|---|
| Separating elements – concrete or masonry | Decrease in thickness and/or density | Not permitted |
| – | Increase in thickness and/or density | Permitted |
| Seal depth | Decrease in seal depth | Not permitted |
| – | Increase in seal depth | Permitted |
| Joint width (W) | Increase in joint width | Interpolation within the tested range between the maximum and minimum nominal joint width is permitted provided the overall seal depth including the backing material is equal or higher |
| – | Decrease in joint width | Permitted |
| Material density | Increase in material density | Not permitted |
| – | Decrease in material density | Not permitted |
| Configuration | Cross section shape of the joint | Permitted only if the area of adhesion remains the same or is increased |
| – | Position of seal within the joint | Distance of the seal from the exposed face in the wall/floor may not be reduced from that tested but may be increased for masonry/concrete walls/floors |
| – | Orientation (H, V) | The classification for vertical linear joints or horizontal linear joints in a vertical test construction (wall) tested without shear movement doesn’t cover other orientations |
| – | Shear movement | The classifications for linear joints in a horizontal test construction (floor) are also valid for a horizontal wall joint abutting a floor, ceiling or roof where shear movement is tested |
| Backing material for sealant seals | Polyurethane/polyethylene | May be interchanged and may be replaced by glass wool, slag wool, stone wool or ceramic wool (the above rules relate to materials of the same or greater depth) |
| – | Stone wool | No change permitted |
| – | Decrease in backing material depth | Not permitted |
| – | Increase in backing material depth | Permitted for Class A1 and A2 materials |
Worked examples of classification
As illustration of the previous concept, the results obtained on a series of linear joints in floors and in walls are provided below.
| Case | Width (mm) | Sealant depth (mm) | Backfilling type | Backfilling depth (mm) | EI | E |
|---|---|---|---|---|---|---|
| 1 | 50 | ≥10 | MW | ≥100 | EI 120-H-X-F-W 50 to W 50 | E 240-H-X-F-W 50 to W 50 |
| 2 | 150 | ≥10 | MW | ≥100 | EI 120-H-X-F-W 150 to W 150 | E 240-H-X-F-W 150 to W 150 |
| 3 | 50 to 150 | ≥10 | MW | ≥100 | EI 120-H-X-F-W 50 to W 150 | E 240-H-X-F-W 50 to W 150 |
| Shear | Sealant width (mm) | Sealant depth (mm) | Backfilling type | Backfilling depth (mm) | EI | E |
|---|---|---|---|---|---|---|
| 10% | 6 | ≥2 | MW | ≥100 | EI 240-H-M 10-F-W 6 to W 6 | E 240-H-M 10-F-W 6 to W 6 |
| 10% | 50 | ≥2 | MW | ≥100 | EI 180-H-M 10-F-W 50 to W 50 | E 240-H-M 10-F-W 50 to W 50 |
| 10% | 6 to 50 | ≥2 | MW | ≥100 | EI 180-H-M 10-F-W 6 to W 50 | E 240-H-M 10-F-W 6 to W 50 |
Case 1 describes a linear joint of 50mm bite and 10mm depth, which was tested with 100mm mineral wool (MW) backfilling without shear movement in a floor. The linear joint resisted 120min in insulation and 240min in integrity E. The classification describes the testing parameters: horizontal floor application (H), no movement tested (X) for bites (W) of 50mm, on field application (F). Therefore, the joint has the classification EI 120-H-X-F-W 50 to W 50 and E 240-H-X-F-W 50 to W 50. The rules allow increasing the depth of 10mm sealant and increasing the backfilling (mineral wool) depth or its density and compression. The same classification can be obtained for Case 2 which has different bite dimensions and as a range of bite dimensions are tested, with a minimum and maximum value, all intermediate values are extrapolated and have the same classification (case 3). As the joint with 150mm also reached 120 minutes in EI and 240minutes in E, a classification for all bites between 50 and 150mm is obtained: EI 120-H-X-F-W 50 to W 150 and E 240-H-X-F-W 50 to W 150.
When joints are tested with shear movement, for example 10%, an additional code M appears in the classification. As can be seen from above table extract, the 6mm wide joint passes 240min insulation whilst the 50mm wide joint only reaches 180min insulation. Therefore, the classification for the range of sealant widths between 6 and 50mm is 180min, the highest commonly reached value.
Similar rules can be applied for the penetration seals and are described in EN15882-3. As a rule of thumb, changes to the build-up which are helping the joint to reach or maintain a certain fire resistance will be allowed. For instance, the sealant and backing depth can be increased or the penetration size decreased. Extrapolation rules related to cables type and positioning are more complex and require careful review.
More technical resources
For supply, quotations and technical questions on DOWSIL™ fire rated sealants, contact us. Source: Dow technical manual (Form No. 62-2233-01-0325 S2D, © 2025 The Dow Chemical Company).